EN 10216-2:2024 specifies technical delivery conditions for seamless non-alloy and alloy steel tubes with specified elevated-temperature properties, replacing EN 10216-2:2013+A1:2019. It covers two test categories and supports compliance with the EU Pressure Equipment Directive 2014/68/EU. Common grades include P195GH, P235GH, P265GH, 16Mo3, 13CrMo4-5, and 10CrMo9-10 for boilers, superheaters, steam lines, heat exchangers, and high-temperature process piping. Base selection on design pressure, operating temperature, wall thickness, delivery condition, inspection category, and elevated-temperature proof strength. Verify chemical composition, mechanical properties, heat treatment, dimensional tolerances, hydrostatic testing, and nondestructive examination before ordering.
Overview of EN 10216-2:2024 and Its Scope
EN 10216-2:2024 is a European standard specifying technical delivery conditions for seamless steel tubes used in pressure applications. Full title: Seamless Steel Tubes for Pressure Purposes – Technical Delivery Conditions – Part 2: Non-Alloy and Alloy Steel Tubes with Specified Elevated Temperature Properties.
Establishes requirements for: material quality, chemical composition, mechanical properties, manufacturing, inspection, and testing.
Typical applications: power plant boilers, steam pipelines, heat exchangers, petrochemical facilities, industrial pressure equipment.
Quick Overview
| Aspect | Key Point |
|---|---|
| Standard | EN 10216-2:2024 |
| Product | Seamless steel tubes for pressure purposes |
| Material categories | Non-alloy steel, alloy steel |
| Test categories | TC1, TC2 |
| Supersedes | EN 10216-2:2013+A1:2019 |
| Not a design code | Does not independently determine max allowable temperature/pressure |
1. Scope of Application
Primarily applies to seamless steel tubes with circular cross-section—manufactured from non-alloy and alloy steels with specified elevated-temperature properties.
Non-circular cross-sections may also be applied when necessary modifications are agreed during enquiry and ordering.
| Material Category | Common Grades | Key Characteristic |
|---|---|---|
| Non-alloy steel tubes | P195GH, P235GH, P265GH | Used in pressure systems requiring suitable strength and mechanical properties at elevated temperatures |
| Alloy steel tubes | 16Mo3, 13CrMo4-5 | Alloying elements improve high-temperature strength and resistance to long-term thermal stress—commonly considered for demanding boiler and industrial piping |
Appropriate grade depends on: operating temperature, design pressure, wall thickness, service conditions, and relevant engineering requirements.
2. Test Categories: TC1 and TC2
EN 10216-2 includes two test categories—defining different levels of inspection and testing.
| Category | Key Point |
|---|---|
| TC1 | Basic inspection and testing requirements |
| TC2 | More extensive inspection and testing requirements than TC1 |
For non-alloy steel tubes: applicable test category must be specified when placing an order.
Important: Test category should not be confused with steel grade—it determines inspection requirements rather than basic material classification. Confirm required category according to project specification, pressure equipment design, and applicable regulations.
3. Relationship with the Previous Edition
EN 10216-2:2024 supersedes EN 10216-2:2013+A1:2019.
| Detail | Key Point |
|---|---|
| Approval | Approved by CEN on October 13, 2024 |
| Publication | Published in November 2024 |
| Content | Technical revisions to material, testing, and delivery requirements |
For buyers: new procurement documents should clearly identify the required edition. Existing projects may still refer to the previous edition—follow contractual requirements rather than changing specifications without engineering approval.
4. What the Standard Does Not Determine
Important: EN 10216-2:2024 is a product standard—not a complete pressure equipment design code.
| Standard Does | Standard Does Not |
|---|---|
| Specifies tube delivery and quality requirements | Independently determine maximum allowable operating temperature or pressure for every application |
| Defines material, testing, and inspection requirements | Guarantees suitability for every high-temperature environment |
These limits must be established through: engineering calculations, material data, applicable design codes, and project-specific conditions.
Compliance with EN 10216-2 does not automatically guarantee suitability for every high-temperature environment. Verify the selected grade, delivery condition, dimensions, and required testing before ordering.
Common Steel Grades and Their High-Temperature Applications
Steel grade selection is a key factor when purchasing seamless steel tubes under EN 10216-2:2024. Different grades have different chemical compositions, mechanical properties, and resistance to elevated temperatures.
EN 10216-2:2024 covers both non-alloy and alloy steel tubes with specified elevated-temperature properties.
Common Steel Grades Comparison
| Steel Grade | Material Category | Typical Applications |
|---|---|---|
| P195GH | Non-alloy steel | General pressure equipment and piping |
| P235GH | Non-alloy steel | Boilers, heat exchangers, pressure pipelines |
| P265GH | Non-alloy steel | Pressure vessels and industrial piping |
| 16Mo3 | Molybdenum-alloy steel | Boilers, steam pipelines, heat exchangers |
| 13CrMo4-5 | Chromium-molybdenum steel | Boiler systems and high-temperature pipelines |
| 10CrMo9-10 | Chromium-molybdenum steel | Power plants and high-temperature pressure equipment |
| 11CrMo9-10 | Chromium-molybdenum steel | Demanding high-temperature pressure applications |
| 14MoV6-3 | Molybdenum-vanadium alloy steel | High-temperature power generation equipment |
Other grades such as 20MnNb6, 10CrMo5-5, and 25CrMo4 are also covered by the standard.
1. Common Non-Alloy Steel Grades
Widely used in boilers, pressure vessels, heat exchangers, and industrial piping—offer a practical combination of mechanical strength, weldability, and cost efficiency.
| Grade | Key Characteristic |
|---|---|
| P195GH | Moderate mechanical strength—suitable for pressure equipment and piping under specified temperature conditions |
| P235GH | Balance of strength, formability, and weldability—wide range of industrial applications |
| P265GH | Higher specified room-temperature strength than P195GH and P235GH—used where design requires corresponding mechanical properties |
These grades are not interchangeable. Compare specified mechanical properties and elevated-temperature data before selection.
2. Common Alloy Steel Grades
Often selected for more demanding high-temperature applications—elements such as chromium and molybdenum improve resistance to high-temperature degradation and support strength retention.
| Grade | Key Characteristic |
|---|---|
| 16Mo3 | Molybdenum-alloy steel—suitable for applications requiring improved elevated-temperature properties compared with many conventional non-alloy steels |
| 13CrMo4-5 | Chromium-molybdenum alloy steel—supports high-temperature strength and resistance to certain forms of thermal degradation |
| 10CrMo9-10 | Chromium-molybdenum steel—associated with more demanding high-temperature pressure applications |
| 11CrMo9-10, 14MoV6-3 | Alloy steel designations encountered in European high-temperature engineering—applicability under EN 10216-2:2024 should be checked against exact grade list and project documentation |
3. How Alloying Elements Improve High-Temperature Performance
| Element | Contribution |
|---|---|
| Molybdenum (Mo) | Improves high-temperature strength and resistance to creep deformation |
| Chromium (Cr) | Improves oxidation resistance; contributes to high-temperature strength |
| Vanadium (V) | Improves strength and microstructural stability through carbide formation |
| Manganese (Mn) | Contributes to strength and hardenability; supports overall mechanical properties |
Effectiveness depends on: concentration, heat treatment, and complete chemical composition. Alloy content alone should not be used to determine material suitability.
4. Selecting Steel Grades for High-Temperature Applications
Consider more than room-temperature tensile strength.
| Factor | What to Evaluate |
|---|---|
| 1. Operating temperature | Elevated-temperature proof strength of selected grade |
| 2. Working pressure | Tube dimensions and material properties meet design requirements |
| 3. Long-term service conditions | Creep resistance and relevant creep rupture data—where prolonged high-temperature exposure is expected |
| 4. Manufacturing & heat treatment | Delivery condition meets requirements for selected grade |
| 5. Project specifications | Required inspection category, testing options, and documentation |
Examples:
- P235GH and P265GH — commonly considered for general pressure applications
- 16Mo3 and 13CrMo4-5 — frequently used in boiler and high-temperature piping systems
- More demanding conditions — may require other alloy grades—depending on engineering calculations and applicable design codes
Key High-Temperature Performance Requirements
High-temperature performance is one of the most important considerations when selecting seamless steel tubes under EN 10216-2:2024. Tubes used in boilers, steam pipelines, heat exchangers, and petrochemical equipment must withstand internal pressure while maintaining sufficient mechanical strength at elevated temperatures.
Unlike ordinary room-temperature specifications, EN 10216-2:2024 addresses elevated-temperature proof strength and provides information on creep rupture strength.
Key Performance Requirements at a Glance
| Requirement | Key Point |
|---|---|
| 1. Elevated-temperature proof strength (Rp0.2) | Minimum values at different temperatures; Option 6 for testing verification |
| 2. Room-temperature tensile properties | Yield strength (ReH), tensile strength (Rm), elongation (A) |
| 3. Creep resistance | Long-term performance under sustained high-temperature stress |
| 4. Creep rupture strength | Informational values in Annex A—not guaranteed minimums |
| 5. Oxidation resistance & thermal stability | Depends on composition, temperature, atmosphere, exposure time |
1. Elevated-Temperature Proof Strength
Rp0.2 indicates the stress required to produce 0.2% permanent deformation at a particular temperature. As temperature increases, strength of most steel materials decreases—a tube meeting room-temperature requirements may have significantly lower load-bearing capacity at high temperature.
Minimum Rp0.2 values from Table 5 (MPa):
| Steel Grade | 300°C | 400°C | 450°C |
|---|---|---|---|
| P235GH | 132 | 112 | 108 |
| P265GH | 154 | 134 | 128 |
| 16Mo3 | 173 | 156 | 150 |
| 13CrMo4-5 | 192 | 174 | 168 |
Values from Table 5 for specified wall-thickness ranges.
Important purchasing detail — Option 6: If purchaser specifies this option—elevated-temperature proof strength must be verified by testing. Test temperature must be agreed upon and specified during enquiry and ordering.
Do not confuse Table 5 values with a requirement to test every delivered tube at every listed temperature.
2. Room-Temperature Tensile Properties
Although high-temperature performance is the main focus, room-temperature mechanical properties remain essential. EN 10216-2:2024 specifies requirements in Table 4.
| Indicator | Key Point |
|---|---|
| Yield strength (ReH) | Stress at which material begins to deform plastically |
| Tensile strength (Rm) | Maximum stress material can withstand during tensile test |
| Elongation (A) | Material’s ductility and ability to deform before fracture |
Required values depend on steel grade and wall thickness. Check relevant standard tables—do not apply one set of properties to all grades.
3. Creep Resistance and Long-Term Performance
Creep is the gradual and permanent deformation of a material under sustained stress—particularly at elevated temperatures for long periods.
For boiler tubes, steam pipelines, and power plant equipment: creep resistance is important—components may operate continuously under high temperature and pressure. Excessive creep deformation can: gradually reduce wall thickness, affect dimensional stability, and eventually contribute to failure.
Chromium-molybdenum alloy steels (13CrMo4-5, 10CrMo9-10) are commonly considered for improved high-temperature performance—suitability must be evaluated using relevant material data and design conditions.
4. Creep Rupture Strength
Describes the stress a material can withstand at a specified temperature for a defined period before rupture occurs.
EN 10216-2:2024 provides creep rupture strength values in Annex A for informational purposes. These values help engineers assess long-term material behavior—but should not be treated as guaranteed minimum properties for every delivered tube.
For actual equipment design: consider applicable design codes, material assessment methods, operating conditions, and required service life.
5. Oxidation Resistance and Thermal Stability
High-temperature steel tubes may experience oxidation, thermal cycling, and microstructural changes during service.
| Consideration | Key Point |
|---|---|
| Oxidation resistance | Chromium-containing alloy steels generally offer better resistance than many conventional carbon steels—depends on complete chemical composition, temperature, atmosphere, and exposure time |
| Thermal cycling | Heating and cooling rates should be considered |
| Process media | Possibility of corrosion from process media |
EN 10216-2 compliance alone does not guarantee resistance to every high-temperature corrosion environment.
6. Key Factors for Material Selection
| Factor | What to Evaluate |
|---|---|
| 1. Operating temperature | Relevant elevated-temperature proof strength values |
| 2. Design pressure | Selected grade and dimensions meet pressure design requirements |
| 3. Service duration | Creep and creep rupture behavior for long-term applications |
| 4. Chemical environment | Oxidation, corrosion, and process-media compatibility |
| 5. Inspection requirements | Additional testing—including Option 6 where elevated-temperature proof strength verification is required |
Manufacturing, Heat Treatment, and Quality Inspection Requirements
The manufacturing process, heat treatment, and quality inspection of seamless steel tubes directly affect mechanical properties, dimensional accuracy, and high-temperature performance.
Under EN 10216-2:2024, seamless tubes for pressure applications must meet specified requirements for manufacturing quality, chemical composition, mechanical properties, and testing.
Key Requirements at a Glance
| Area | Key Requirements |
|---|---|
| 1. Manufacturing process | Billet preparation → heating → piercing → rolling/elongation → sizing → cooling/inspection |
| 2. Heat treatment | Normalizing, normalizing & tempering, quenching & tempering, stress-relieving—per grade and delivery condition |
| 3. Chemical & mechanical testing | Composition analysis, tensile testing, impact testing (as required), elevated-temperature proof testing (when specified) |
| 4. NDT & dimensional inspection | UT, electromagnetic testing, visual inspection, dimensional checks, hydrostatic testing (where required) |
| 5. Certificates & traceability | EN 10204 Type 3.1 certificate; heat number, test results, heat treatment records |
1. Seamless Steel Tube Manufacturing Process
Manufactured without a longitudinal weld seam.
| Stage | Action |
|---|---|
| 1. Billet preparation | Steel billets selected per grade and chemical composition; surfaces inspected before heating |
| 2. Heating | Billets heated to suitable temperature—achieve plasticity required for hot working |
| 3. Piercing | Rotary piercing creates hollow shell from solid billet |
| 4. Rolling & elongation | Hollow shell rolled to required outside diameter and wall thickness |
| 5. Sizing & finishing | Tube passes through sizing or reducing equipment—obtain specified dimensions |
| 6. Cooling & inspection | Tubes cooled under controlled conditions; checked for surface defects and dimensional accuracy |
Exact production route may vary—depending on steel grade, tube dimensions, and manufacturing equipment. Proper process control is essential for consistent wall thickness, mechanical properties, and structural integrity.
2. Heat Treatment Requirements
Helps establish required microstructure and mechanical properties—while reducing residual stresses from hot working or subsequent processing.
| Treatment | Purpose |
|---|---|
| Normalizing | Refines grain structure; helps produce consistent mechanical properties |
| Normalizing & tempering | Combines structural refinement with improved strength and toughness |
| Quenching & tempering | Used for applicable alloy steel grades—achieve specified combination of strength and toughness |
| Stress-relieving | May be required for particular manufacturing or service conditions when specified |
Required heat treatment condition depends on individual steel grade and standard’s delivery requirements. Confirm delivery condition when placing an order—verify through inspection documentation.
3. Chemical Composition and Mechanical Testing
Chemical composition determines basic characteristics—including strength, weldability, and high-temperature performance. EN 10216-2:2024 specifies limits for each grade.
| Verification Activity | Key Point |
|---|---|
| Chemical analysis | Carbon, manganese, silicon, other alloying elements |
| Alloy grade verification | Chromium and molybdenum content for relevant grades |
| Room-temperature tensile testing | Per standard requirements |
| Impact testing | Where required by selected grade and test category |
| Elevated-temperature proof strength testing | When specified by purchaser |
For 16Mo3 and 13CrMo4-5: particular attention to alloying element content—contributes to high-temperature properties.
4. Non-Destructive Testing and Dimensional Inspection
| Inspection Method | Purpose |
|---|---|
| Ultrasonic testing (UT) | Detect internal imperfections and certain discontinuities |
| Electromagnetic testing | Identify relevant defects in suitable tube products |
| Visual inspection | Check surface condition, visible defects, finishing quality |
| Dimensional inspection | Verify outside diameter, wall thickness, length, straightness, other tolerances |
| Hydrostatic testing | Verify pressure integrity—where required |
Applicable testing method and acceptance requirements depend on the standard, test category, and order specifications.
5. Inspection Certificates and Traceability
Material traceability is particularly important for pressure equipment in high-temperature environments.
EN 10204 Type 3.1 inspection certificate is commonly requested for pressure-service steel tubes—provides test results and confirms compliance with order requirements through manufacturer’s authorized inspection representative.
| Purchaser Should Check | Key Point |
|---|---|
| Steel grade & standard edition | Per order requirements |
| Heat number & product identification | Traceability records |
| Chemical composition results | Per standard requirements |
| Mechanical test results | Per standard requirements |
| Heat treatment condition | Delivery condition verification |
| NDT & hydrostatic test records | Where applicable |
| Dimensional inspection results | Per order requirements |
How to Select EN 10216-2:2024 Seamless Steel Tubes for Different Applications
Selecting the right seamless steel tubes under EN 10216-2:2024 requires careful consideration of operating temperature, design pressure, material properties, and service environment. Choosing an unsuitable grade may increase maintenance costs and affect safety and service life.
Common grades: P195GH, P235GH, P265GH, 16Mo3, 13CrMo4-5, and 10CrMo9-10—each with specific characteristics for different engineering conditions.
Application Selection Guide
| Industry/Application | Recommended Grades | Key Consideration |
|---|---|---|
| Power generation | P235GH, P265GH, 16Mo3, 13CrMo4-5, 10CrMo9-10 | Elevated-temperature proof strength, long-term creep performance |
| Petrochemical | 13CrMo4-5, 10CrMo9-10 | Operating temperature, pressure, process environment; corrosion resistance |
| Chemical plants | P235GH, P265GH; alloy grades where required | Chemical compatibility, welding, pressure equipment regulations |
| Heat exchangers | Per design requirements | Pressure, thermal changes, corrosion, heat transfer |
| Industrial boilers | P235GH, P265GH; 16Mo3, Cr-Mo grades for demanding conditions | Boiler design code, temperature, pressure |
1. Power Generation Applications
Used in boilers, superheaters, steam pipelines, and pressure-bearing components—must withstand high temperatures, internal pressure, and long operating periods.
| Grade | Typical Application |
|---|---|
| P235GH, P265GH | Pressure applications where specified mechanical properties meet design requirements |
| 16Mo3 | Boiler components and steam systems requiring improved elevated-temperature properties |
| 13CrMo4-5, 10CrMo9-10 | More demanding high-temperature applications where alloy composition and mechanical properties are appropriate |
For power generation projects: evaluate elevated-temperature proof strength and long-term creep performance—not just room-temperature tensile properties.
2. Petrochemical Industry
Pressure piping transports steam, process fluids, and other media under varying temperature and pressure conditions.
Chromium-molybdenum alloy steel tubes (13CrMo4-5, 10CrMo9-10) may be suitable for selected high-temperature process applications—check material properties against operating temperature, pressure, and process environment.
For pipelines exposed to corrosive chemicals or aggressive media: also evaluate corrosion resistance. EN 10216-2 compliance alone does not guarantee suitability for every chemical environment.
3. Chemical Plants and Industrial Pressure Equipment
Equipment operates under changing temperatures and pressure conditions—tubes used in reactors, pressure vessels, and associated piping must meet relevant design and material requirements.
| Grade | Application |
|---|---|
| P235GH, P265GH | Suitable non-alloy steel applications |
| Alloy grades | When improved elevated-temperature performance is required |
Confirm before selecting: chemical compatibility, operating conditions, welding requirements, and applicable pressure equipment regulations.
4. Heat Exchanger Applications
Require tubes that withstand internal pressure and repeated thermal changes.
| Selection Consideration | Key Point |
|---|---|
| Operating & design temperatures | Per application requirements |
| Internal & external pressure | Per design conditions |
| Heat transfer | Per thermal requirements |
| Corrosion | Process media characteristics |
| Dimensions | Tube outside diameter and wall thickness |
| Service life | Expected duration and maintenance conditions |
Selected grade must satisfy mechanical and pressure-design requirements. Also evaluate: corrosion resistance and heat transfer performance per specific application.
5. Industrial Boiler Applications
Operate under elevated temperatures and pressure—material selection particularly important.
| Grade | Application |
|---|---|
| P235GH, P265GH | Commonly used for suitable pressure applications |
| 16Mo3, Cr-Mo grades | More demanding thermal conditions |
Final selection should be based on: boiler design code, operating temperature, design pressure, and required material properties—not steel grade alone.
6. Practical Purchasing Checklist
| Purchasing Factor | Key Requirements |
|---|---|
| Steel grade | P235GH, P265GH, 16Mo3, or another specified grade |
| Dimensions | Outside diameter, wall thickness, length |
| Operating conditions | Design temperature and pressure |
| Delivery condition | Required heat treatment and finishing condition |
| Test category | TC1 or TC2, as applicable |
| Mechanical properties | Tensile, impact, elevated-temperature properties where required |
| Inspection | NDT, hydrostatic testing, other specified tests |
| Documentation | Inspection certificate and material traceability |
Our Recommended EN 10216-2 Seamless Steel Tube Products and Global Shipping Services
Supplies EN 10216-2:2024 seamless steel tubes for boilers, superheaters, steam lines, heat exchangers, and high-temperature pressure piping. Available grades include P235GH, P265GH, 16Mo3, 13CrMo4-5, and 10CrMo9-10, covering non-alloy and alloy steels with specified elevated-temperature properties. Orders should confirm outside diameter, wall thickness, length, delivery condition, inspection category, heat treatment, chemical composition, mechanical properties, hydrostatic testing, and non-destructive examination. Export packaging, corrosion protection, commercial invoices, packing lists, and shipping coordination are arranged to confirm order requirements. Provide grade, dimensions, quantity, destination port, and applicable PED/EN requirements to request a quotation.
Conclusion:
Selecting EN 10216-2:2024 seamless steel tubes requires matching material properties with actual operating conditions, not just room-temperature strength. Non-alloy grades such as P195GH, P235GH, and P265GH suit boilers, heat exchangers, and industrial pressure piping, while alloy grades including 16Mo3, 13CrMo4-5, and 10CrMo9-10 support higher-temperature steam and process applications. Confirm elevated-temperature proof strength, design pressure, wall thickness, delivery condition, heat treatment, inspection category, hydrostatic testing, and non-destructive examination before ordering. Proper quality documentation and supplier communication help reduce procurement risks for European pressure-equipment projects.
FAQ:
1. What is EN 10216-2:2024 used for?
It specifies technical delivery conditions for seamless non-alloy and alloy steel tubes used in pressure applications with specified elevated-temperature properties.
2. What is the difference between EN 10216-2:2024 and the previous edition?
The 2024 edition supersedes EN 10216-2:2013+A1:2019 and updates technical requirements for materials, testing, and delivery conditions.
3. Which steel grades are commonly used for high-temperature applications?
Common grades include 16Mo3, 13CrMo4-5, and 10CrMo9-10, depending on operating conditions and design requirements.
4. What is the difference between P235GH and 16Mo3?
P235GH is a non-alloy pressure steel, while 16Mo3 is a molybdenum-alloy steel commonly used for applications requiring improved elevated-temperature properties.
Post time: Nov-03-2026